Properties
Properties
Mechanical properties
The values shown for the mechanical properties in the table below are for test pieces taken transverse to the rolling direction:
EN 10111: 2008 | Grade | DD11 |
---|---|---|
Yield strength ReL (N/mm2) | 1.5 ≤ t < 2 | 170 - 360 |
2 ≤ t < 11 | 170 - 340 | |
Max. tensile strength Rm (N/mm2) | 440 | |
Elongation (%) | 1.5 ≤ t < 2 | 23 |
2 ≤ t < 3 | 24 | |
3 ≤ t < 11 | 28 | |
Min. bend test diameter | 1t |
Values are for test pieces taken transverse to the rolling direction:
t - material thickness in mm
Lower yield strength or 0.2% proof stress applies.
Test piece length L0 = 80mm for thicknesses <3mm and L0 = 5.65√S0 for thicknesses ≥3mm
Chemical composition
Hot-rolled steel for forming meets the requirements of the cast analysis in the standard as shown in the table below:
EN 10111: 2008 | Grade | DD11 |
---|---|---|
C | Max. | 0.12 |
Mn | Max. | 0.6 |
P | Max. | 0.045 |
S | Max. | 0.045 |
Not in EN 10111: 2008. Tata Steel’s own specification.
All values are in weight%.