Properties

Mechanical properties

The mechanical properties are measured transverse to the rolling direction:

 

Relationship with European standard

ReH / Rp

Rm

A80

Adp5

EN 10025-2: 2004, S235JR

N/mm²

N/mm²

%

%

     

t < 3

t ≥ 3

Hot-rolled flat products

≥ 235

360 - 510

≥ 17

≥ 24

 

Ymagine S1

Rp

Rm

A80

Adp5

 

N/mm²

N/mm²

%

%

     

t < 3

t ≥ 3

Typical value

300

395

28

-

Guaranteed values

235 - 360

360 - 510

≥ 19

24

 

Chemical composition

Cast analysis in weight percentages:

Ymagine S1

C

Mn

P

S

Si 1

Typical

0.045

0.220

0.008

0.007

0.018

Guaranteed (max)

0.065

0.300

0.025

0.015

0.035

1. For the purpose of batch galvanising, Ymagine S1 can be ordered on consultation with a maximum Si content of 0.030%.